Welding Procedure Specification: Complete WPS Guide [2026]

A welding procedure specification is the backbone of your welding operation, controlling how every qualified weld is made – the procedure, materials, parameters, and tests used to turn an as-delivered joint into a code-conforming weld. A weld procedure specification that is not written and qualified correctly is an insurmountable barrier to re-assurance from any inspector, contractor, or auditor that a weld will perform adequately in-service.

In this guide we will walk through the full WPS lifecycle: what a welding procedure specification contains, how it differs from a Procedure Qualification Record (PQR), which code specification applies to your work, and how robotic welding makes WPS documents even more important – not less. Whether you are writing your first section IX compliant WPS or reviewing a world class AWS D1.1:2025 prequalified WPS, this guide covers it all.

WPS Quick Reference

Document Type Formal written welding standard (instruction document)
Governing Bodies ASME Section IX, AWS D1.1:2025, ISO 15614-1, API 1104
8 Essential Sections Joint, base metal, filler, preheat, electrical parameters, position, PWHT, testing
Supported Processes SMAW, GMAW, FCAW, GTAW, SAW, PAW, and hybrid combinations
Qualification Path pWPS → test coupon → PQR → certified WPS
Validity Valid until an essential variable changes beyond qualified range

What Is a Welding Procedure Specification (WPS)?

What Is a Welding Procedure Specification (WPS)?

A welding procedure specification sets out repeatable parameters for how an individual weld must be made in order to ensure quality. If you think of it as a recipe, then a WPS specifies the recipe for fabricating a joint: it defines in detail the process which can be used, what base metals and filler metals are allowed, at what settings to operate, in which directions the weld can be made, and what tests are required afterwards to prove the weld is defect free.

The American Welding Society standard AWS B2.1/B2.1M:2021 defines a WPS as “a written document that provides direction to the welder or welding operator for making production welds in accordance with Code requirements.” Bear in mind the caveat “in accordance with Code requirements” — a WPS is not a suggestion. Under the ASME Boiler and Pressure Vessel Code, AWS D1.1 Structural Welding Code, and ISO 15614 internationally, a WPS is a mandatory pre-condition for certified production welding.

Why does this documentation matter at scale? The Welding Institute (TWI) conducted an industry survey of weld repair rates across sectors: average repair rates for Oil & Gas and Power industries range from 1 to 3%, with peak rates reaching 25% in specific locations and exceptional values documented at 55% in the worst cases. The major contributing factors are welder skill variability, weld accessibility, and poor joint fit-up prior to welding. A well-written, well-followed WPS directly addresses welder variability — it removes guesswork from the equation and sets a repeatable floor for weld quality.

💡 Do You Always Need to Write Your Own WPS?

Not always. The American Welding Society publishes Standard Welding Procedure Specifications (SWPS) — prequalified procedures for common applications using carbon steel, stainless steel, and aluminium. SWPSs are backed by published PQR data, which means a shop can adopt an SWPS and skip the testing phase entirely — provided the application falls within the SWPS’s defined scope. This is a significant time and cost saving that many smaller fabricators do not know about.

Essential point to understand: a welding procedure specification is not an optional quality tool but a required instruction set. Its goal: to make certified production welding generic while also removing wet-blowing supervision variation.

WPS vs. PQR vs. WPQR — Understanding the Document Chain

WPS vs. PQR vs. WPQR — Understanding the Document Chain

The three terms — WPS, PQR, and WPQR — are often used interchangeably in the field, but they are distinct documents serving different roles in the welding qualification process. Getting them mixed up is one of the fastest ways to fail a quality audit.

Document What It Is Who Uses It
WPS
Welding Procedure Specification
The instruction document. Tells the welder exactly how to make the weld: process, materials, parameters, position, preheat. Welder, supervisor, inspector — daily production reference
PQR
Procedure Qualification Record
The test record. Documents the actual parameters used during a qualification test weld, plus the destructive/NDT test results that confirm the procedure produces sound welds. Welding engineer, auditor, third-party inspector — qualification evidence
WPQR
Welding Procedure Qualification Record
The European/ISO equivalent of a PQR under ISO 15614-1. Used in EN-standard projects (European, UKCA, international). European inspectors, notified bodies, EN-standard projects

The 4-Stage WPS Qualification Method

The WPS qualification procedure is based on a 4 step sequence within ASME Section IX and AWS D1.1. It is important to master this procedure prior to writing your first WPS:

  1. Draft a pWPS(Preliminary WPS)- Once the welding is planned then draft a welding procedure in advance, with all the essential and non-essential variables set at their planned production values.
  2. Weld a test coupon – Perform the pWPS conditions on a test plate or pipe coupon with the actual production materials using an approved welding operator.
  3. Test & record (PQR) – Destructively test (tensile, bend, impact) & non- destructively test ( radiographic, ultrasonic, visual) test coupon, and document actual parameters and test results in the Procedure Qualification Record.
  4. Issue the certified WPS – if the PQR results satisfy the Code, then produce the production WPS from this PQR as reference. This WPS becomes the contractual document for production fabrication.

Key takeaway: The WPS and PQR are inseparable — the WPS is the instruction, the PQR is the proof. A WPS with no referenced PQR is not a qualified welding procedure under ASME or AWS Code (unless it is an approved SWPS).

What’s Inside a WPS? The 8 Essential Sections

What's Inside a WPS? The 8 Essential Sections

A compliant welding procedure specification must document every variable that could affect the mechanical properties and integrity of the finished weld. The Canadian Welding Bureau (CWB) Welding Procedure Guide — one of the most detailed open references on WPS documentation — organises the required content into eight sections. Each section has a corresponding set of common errors that auditors frequently catch in the field.

  • 1.
    Joint Design — type (butt, fillet, groove), groove angle, root opening, backing material, and fit-up tolerances. Common error: tolerances not specified, allowing welders to fit up outside qualified range.
  • 2.
    Base Metal — material specification, P-Number group, thickness range, and diameter range (pipe). Common error: P-Number not specified, making the WPS ungroupable under ASME IX.
  • 3.
    Filler Metal — AWS classification, F-Number, A-Number, trade name, and flux designation (SAW). Common error: only trade name listed without AWS classification or A-Number — inadequate for audit purposes.
  • 4.
    Preheat and Interpass Temperature — minimum preheat temperature, maximum interpass temperature, and measurement method. Common error: preheat field left blank or entered as “ambient” — this creates a code violation and liability exposure.
  • 5.
    Electrical Parameters — current type (AC/DC), polarity, amperage range, voltage range, wire feed speed (GMAW), and electrode/wire diameter. Common error: ranges too wide (e.g., 90–430 amps, 18–32 volts) — creates a document that is technically compliant but operationally useless.
  • 6.
    Welding Position — qualified position(s) (1G/2G/3G/4G/5G/6G for groove; 1F–4F for fillet), weld progression (up or down for verticals). Common error: position field left blank — welder believes the WPS covers all positions, but it only covers tested ones.
  • 7.
    Post-Weld Heat Treatment (PWHT) — temperature range, hold time, heating/cooling rate. Required for pressure-vessel-class welds on materials prone to hydrogen embrittlement. Common error: PWHT section left blank when it is actually required — ASME Code violation for P4/P5 materials.
  • 8.
    Nondestructive Examination (NDE) & Testing — visual, radiographic, ultrasonic, penetrant, or magnetic particle testing requirements and acceptance criteria. Common error: NDE type listed without acceptance standard (e.g., “RT” without specifying ASME V or API 1104 acceptance criteria).
⚠️ Field Reality Check

But industry people I have spoken to say they have encountered a WPS written to meet a certain customer or local department of commerce audit, then simply filed away in an office never to be posted at the weld station. A WPS a welder has never read is a compliance document not a quality tool. The best WPS programs have a printed sign-off of the welder having read the procedure prior to production.

Essential Variables vs. Non-Essential Variables — When Re-Qualification Is Required

Essential Variables vs. Non-Essential Variables — When Re-Qualification Is Required

Every welding code distinguishes between essential variables — changes that fundamentally alter the mechanical properties of the weld — and non-essential variables — changes that affect the procedure but not weld integrity. Under ASME BPVC Section IX, a change to any essential variable beyond its qualified range requires a new Procedure Qualification Record (PQR) — meaning a new test coupon, new destructive testing, and a new WPS. A change to a non-essential variable requires only a WPS revision, not re-testing.

The ASME Section IX P/F/A-Number System

ASME IX grouped important variables into three systematic schemes intended to avoid duplicated testing in order to minimise tests while still to safeguarding the metallurgical properties:

Variable What It Groups ASME Table Re-qual Trigger
P-Number Base metals by weldability & chemistry
P1 = carbon steel; P8 = austenitic SS
QW-422 Any change from one P-Number to another requires new PQR
F-Number Filler metals by usability skill
F4 = low-hydrogen (E7018); F6 = stainless
QW-432 Change upward (F3→F4) requires new PQR; welder qualified at F4 covers F1–F3
A-Number Deposited weld metal by chemical analysis
A1 = plain carbon; A8 = austenitic SS
QW-442 Any shift in Cr, Mo, or Ni content that changes A-Number requires new PQR

📐 Engineering Note: The A-Number Trap

Experienced welding engineers frequently encounter junior engineers who assume A-Number is based on the filler metal’s trade name or AWS classification. It is not. The A-Number reflects the deposited weld metal chemical composition — determined either from the filler metal manufacturer’s certificate of conformance or, more reliably, from a chemical analysis of the actual PQR test coupon per ASME Table QW-442. When shielding gas composition changes significantly (e.g., switching from 75/25 Ar/CO₂ to pure CO₂), alloying element burnout can shift the deposit composition enough to change the A-Number — potentially invalidating the WPS during a third-party audit.

Re-Qualification Decision Tree

Does My Process Change Require a New PQR?

  1. Does the change affect P-Number? (different base metal group) → YES → New PQR required
  2. Does the change affect F-Number or A-Number? (different filler metal chemistry or usability class) → YES → New PQR required
  3. Does the change involve PWHT addition or removal? (e.g., adding stress relief on P4 material) → YES → New PQR required
  4. Does the change exceed the qualified thickness range? (outside 1T/2T qualified limits) → YES → New PQR required
  5. Is the change limited to travel speed, pass sequence, or electrode diameter within the same F/A-Number? → WPS revision only — no new PQR

A practical example from the field: a piping contractor planned separate qualification tests for SA-106 Grade B (carbon steel) and SA-333 Grade 6 (low-temperature carbon steel). An engineer reviewing ASME Section IX Table QW-422 identified that both materials are classified as P-Number 1. With the same E7018 electrode (F-Number 4, A-Number 1), a single PQR covered both base metals — eliminating approximately ten days of testing time and roughly $4,500 USD in laboratory costs.

The most recent additive changes to ASME BPVC Section IX 2025 edition were: increased qualification coverage of Vertical (V) position, update of essential variable requirements of Duplex Stainless Steel- see the current edition if your work applies to these materials,

WPS by Standard — ASME IX, AWS D1.1, ISO 15614, and API 1104 Compared

WPS by Standard — ASME IX, AWS D1.1, ISO 15614, and API 1104 Compared

Picking the incorrect governing code for a WPS is a project level mistake it can invalidate qualification testing done under the wrong code and mean that the project has to re-qualify at its own cost. The four existing major international welding standards cover different areas of use and their scope boundaries can sometimes be quite confused:

Standard Jurisdiction Primary Application Key WPS Requirement
ASME BPVC Section IX USA, international (ASME-stamp projects) Boilers, pressure vessels, power piping — anywhere an ASME Code stamp is required PQR mandatory; P/F/A-number system; mandatory PWHT documentation for qualifying materials
AWS D1.1:2025 USA structural fabrication Structural steel — buildings, bridges, industrial platforms, cranes, mining structures Prequalified WPS option (no PQR needed if all conditions met); 2025 edition adds A913 Grade 80 as prequalified base metal and LRFD methodology
ISO 15614-1 Europe, international (EN-standard projects) All fusion-welded metallic structures — functional equivalent of ASME IX outside North America; WPQR format used instead of PQR WPQR mandatory; grouping system follows ISO/TR 15608 (material groups) instead of ASME P-Numbers
API 1104 USA, international (pipeline projects) Oil and gas pipelines — onshore and offshore transmission pipelines Separate WPS qualification from ASME IX — PQR must be pipeline-specific; cellulosic and low-hydrogen electrode distinctions are essential variables; radiographic acceptance per API 1104 Appendix A

Standards Selection Matrix — Which Code Applies to My Project?

If your application is…

  • Power generation boiler/pressure vessel ASME BPVC Section IX (Required if ASME Code stamp obtained)
  • Steel building, bridge, or industrial facility AWS D1.1:2025; may use prequalified WPS to avoid PQR testing
  • A European or international project is being designed according to EN standards ISO 15614-1producing a WPQR rather than a PQR
  • Oil or Gas pipeline API 1104; be aware that ASME IX qualification is not transfer able – you’ll need to be re-qualified if applying for this.
  • Project crosses several codes LC Number is chose to be the most restrictive. Go to the CWI or Welding Engineer first before beginning a ‘qualification’ programme.

A practical note on 2025 code updates: AWS D1.1:2025 (the 25th edition) introduced the addition of A913 Grade 80 as a prequalified base metal — the highest yield-strength material ever approved for prequalification under D1.1 at 80 ksi minimum yield. If your structural project uses high-strength steel and you were previously forced into full PQR qualification, the 2025 edition may now allow prequalified status. Check the current edition before beginning any new qualification programme, as using an outdated code edition can result in rejected welds on a contract that references the current standard.

WPS Parameters for GMAW, GTAW, and SAW — A Process Reference

WPS Parameters for GMAW, GTAW, and SAW — A Process Reference

What Are the Essential Parameters in a MIG (GMAW) Welding Procedure Specification?

Each process has processing parameter requirements, then the process parametric value has to be listed in the well-qualified WPS. The table is about the process-level guidance to the three most popularly used industrial processes in structural and pressure vessels fabrication: GMAW/MIG, GTAW/TIG and SAW respectively. The values are summarized from many industrial references like the CWB Welding Procedure Guide and various industry references; you will need different optimum values in your specific application depending on material grade, thickness, position and equipment.

Always check with your welding engineer.

Parameter GMAW (MIG) GTAW (TIG) SAW
Current Type DCEP (DC+) DCEN (DC−) or AC (aluminium) DCEP or AC (multi-wire)
Typical Current Range (carbon steel) 100–350 A 60–200 A 300–700 A
Typical Voltage Range 17–28 V 10–15 V (arc gap) 28–42 V
Shielding Gas / Flux 75/25 Ar/CO₂ or 100% CO₂
Flow: 25–45 CFH (CWB)
100% Argon (steel/Ti); 75/25 Ar/He (thick aluminium)
Flow: 15–20 CFH (CWB)
Granular flux (no shielding gas); flux classification per AWS A5.17
Wire/Electrode Diameter 0.035″–0.062″ (0.9–1.6 mm) 1/16″–3/32″ tungsten; filler wire 1/16″–3/32″ 5/64″–1/4″ wire; 3/32″ common for structural
Wire Feed Speed (WFS) 200–600 in/min (5–15 m/min) Manual wire feed (speeds vary) 50–150 in/min depending on wire diameter
Transfer Mode (GMAW) Spray (>26V), Globular, Short-circuit, Pulse N/A N/A (submerged arc)
Best For Structural steel, automation, high-deposition fabrication; prequalified under AWS D1.1 (spray only) Root passes, precision joints, stainless, titanium, thin-gauge material Heavy-section butt and fillet welds; boiler drums, pressure vessels, ship hulls

📐 Engineering Note: Heat Input Calculation

Heat input is also an important essential variable under ASME Section IX it manages the heat affected zone (HAZ) width and the cooling rate, that will affect the mechanical properties and toughness of the weld. The standard equation is:

H = (V × A × 60) / (1000 × T)

Where H = heat input (kJ/mm), V = arc voltage (volts), A = welding current (amps), T = arc travel speed (mm/min). Example: welding a 12 mm carbon steel boiler plate at 24 V, 220 A, 250 mm/min travel speed → H = (24 × 220 × 60) / (1000 × 250) = 1.27 kJ/mm. Exceeding the qualified maximum heat input is an essential variable violation that requires new PQR testing.

⚠️ Important: GMAW Short-Circuit Restriction

Use of GMAW short-circuit transfer for prequalified WPS table 3/4 WPS of AWS D1.1 NOT allowed. Short circuit transfer is susceptible to lack of fusion in groove welds when welding on thicker plate sections. Place of use of GMAW in a WPS for structural groove welds must be proved by testing, use of short-circuit transfer mode cannot be prequalified.

WPS in Automated and Robotic Welding — Why Documentation Matters More, Not Less

WPS in Automated and Robotic Welding — Why Documentation Matters More, Not Less

Do Robotic Welding Systems Still Need a WPS?

A common misconception in automation adoption is that robotic welding reduces the need for WPS discipline. The opposite is true. When a robot executes a weld, it executes that WPS thousands of times at scale — every deviation from the qualified parameters is replicated across every joint, every shift, every week of production. A WPS error that a skilled manual welder might intuitively compensate for becomes a systemic defect in an automated cell.

“Before we installed the robotic cells, our radiographic testing reject rate on pressure vessel seams ran at around 9%. After qualification and integration — with the robot operating within a tightly defined WPS at ±5% parameter tolerance — we brought that figure down to 1.8%. The WPS did not become less important. The robot just enforced it consistently every cycle.”

— Production Supervisor, Henan Boiler Facility (Zhouxiang robotic welding installation, power industry)

That 1.8% radiographic test (RT) reject rate achieved at the Henan Boiler Facility is worth contextualising against industry benchmarks. According to a TWI (The Welding Institute) industry survey, average repair rates for pressure vessels range from 1.1% to 2.8% depending on material grade — with an average across all products of 2.0%. The automated cell, operating within a qualified WPS with real-time parameter monitoring, brought the facility below the global industry average for that product category.

The technical architecture that makes this possible:

  • Zhouxiang robotic cells achieve ±0.05 mm repeat positioning accuracy (per ISO 9283:1998), ensuring torch-to-joint consistency that manual welding cannot replicate across shifts
  • Parameter deviations exceeding ±5% from WPS-specified amperage or voltage trigger an automatic pause, halting the weld before a non-conforming deposit is completed
  • Every weld cycle generates a digital parameter log — date, time, joint ID, actual amperage, voltage, travel speed, and heat input — creating a real-time PQR-equivalent traceability record for ASME compliance

9% → 1.8%
RT Reject Rate (Henan Boiler)
±0.05 mm
Repeat Positioning Accuracy (ISO 9283:1998)
±5%
Parameter Deviation Threshold → Auto-Pause

This architecture reflects a broader shift in how WPS compliance is enforced in automated environments. Traditional manual welding relies on welder skill and periodic inspection to enforce WPS parameters. Robotic welding moves enforcement upstream — into the machine itself — where the WPS parameters are programmed as hard operating limits, not advisory targets.

Digital Traceability and the Future of WPS (2025–2026)

Digital Traceability and the Future of WPS (2025–2026)

Welding procedure compliance is entering a digital-first era. The five shifts identified in Pemamek’s Trends Shaping Welding Automation in 2026 article (published 13 February 2026) reflect an industry moving away from paper-based WPS documentation and toward real-time digital compliance systems.

  1. AI & Adaptive Welding – Closed-loop control systems use sensors and machine learning to adjust welding parameters in real time. Rather than reacting to variation by adjusting by feel, a welder would have their arc length and travel speed corrected by the system as the system notices arc instability. Within a WPS-validated window of tolerance, the process proceeds and the system operates as a rather rigid WPS enforcer.
  2. Digital Twins &Virtual Commissioning – robot trajectories, PLC logic, weld control settings are validated in a digital emulation environment prior to a new welding cell arriving on the shop floor. Changes that would historically mandated costly and time consuming physical test runs can now be assessed virtually. Remote Factory Acceptance Testing (FAT) is increasingly viable for massive international projects.
  3. Laser & Hybrid Welding Expansion – The progression from precision laser applications into heavy fabrication (wind energy assemblies, ship constructing, primary steel erections) presents new, critical process variables (beam power, focus location, standoff) requiring a new framework for laser hybrid WPS qualification. Design teams planning a laser process weld cell installation between 2026 and 2027 should consider inclusion of laser or hybrid laser WPS qualification within the overall project procurement specifications.
  4. Data Based Service Concepts – Upstream, equipment vendors offer guaranteed outcomes (uptime, run rate, weld quality) in lieu of capital cost: IoT-connected cells supply ongoing diagnostic information (drift of production parameters) allowing up-front dashboard alerting of parameter overages that would otherwise result in systematic defects in subsequent production runs – a shift that reduces your inventory carrying costs and time lost in reactive post-production inspection.
  5. Work force Readjustment – the worldwide skilled welder shortfall is fueling automation growth: applications are moving from torch-in-hand to torch-in-automation supervision and WPS maintenance. A fabricator who can write, qualify, and embed a WPS into a robotic cell is commanding a premium over one whose skillset is limited to torch inflow.

Action Recommendation — If You’re Planning 2026–2027 Automation

If your business is planning an industrial automation capital purchase between 2026 and 2027, digital parameter logging linked to the WPS should be a part of your requested purchase specifications – not an aftersales add-on. Request of your robotic welding system provider: (1) real-time parameter logging in an ASME compatible csv or xml, (2) configurable deviation alerting action-sets per WPS, and (3) automatic audit trail production per weld joint. Your WPS-linked system will enable your third-party inspection program to focus on systemic quality control issues rather than third party document checking – ultimately underpinning your digital compliance cases in ASME, AWS, and ISO audits.

Frequently Asked Questions

What are the 5 essential procedures in welding?

View Answer

While KAD 5 essential procedures is not a found code reference – it delineates the five key WPS quality components for a code compliant operation: (1) WPS – the “how to” instruction set; (2) PQR – the document containing the test evidence; (3) WPQ/WPT – the individual’s welder qualification; (4) MTR – base metal adherance to specification; and (5) NDE report – visual, radiographic, or ultrasonic inspection results. These five quality steps are required for each official weld to meet ASME, AWS and ISO authority audit standards.

How do you create a Welding Procedure Specification?

View Answer

WPS creation steps are: (1) the guiding code of use (ASME Section IX, AWS D1.1, ISO 15614, API 1104), (2) generation of a preliminary WPS (pWPS), indicating all essential and non-essential variables before production, (3) validation via destructive and NDE testing testing, (4) implementation of certified WPS including referencing of the test evidence (PQR), (5) Engineering sign off. Common material types and processes covered by AWS Standard Welding Procedure Specification (SWPS) may be eligible to avoid the destructive testing step.

Who is responsible for writing and approving a WPS?

View Answer

The fabricator (shipyard/welding company) must generate and authorise the WPS. Most WPSs are composed by a Certified Welding Inspector (CWI), a Certified Welding Engineer (CWEng) or a senior welding engineer who is familiar with the relevant code. Engineering approval, i.e. a confirmation that the WPS was qualified in accordance with the appropriate code, must be shown on the text.

An approved WPS with no approval signature is not a complete auditing document. Approved third party inspection agencies (authorised inspection authorities under ASME) will perform an review of the WPS and PQR documents however the fabricator will still generate the WPS.

What is the difference between a prequalified and a qualified WPS?

View Answer

A prequalified WPS (which is the WPS available under AWS D1.1 for structural welding) is a procedure which is in compliance with all of the instructions defined in the code as a requirement for prequalification, that is, it uses the prescribed base metals, filler metals, joint geometries, and process parameters, and therefore does not require a test coupon or PQR. A prequalified WPS can be assumed to produce sound welds, since the combination of material and process has been tested rather than a specific application. A qualified WPS (a reference requirement in ASME Section IX, API 1104, and whenever the procedural application does not meet the prescribed prequalified conditions in D1.1) requires the welding of a test coupon to be produced and tested prior to the WPS being used.

A prequalified WPS can reduce the expense of testing each weld, but only when the code instructions are followed. Some violations seen historically are GMAW short-circuit transfer, use of incorrect groupings, and large single pass weld sizes.

How long is a WPS valid?

View Answer

A certified WPS has no time limit according to ASME Section IX or AWS D1.1 – it remains ‘qualified’ for indefinite period of time provided no ‘essential variables’ are changed beyond their qualified range. The validity of a WPS is based on stability of essential variables not on specific time limits. The WPS will need to be re-qualified (new PQR required) if: the base P-Number limits are exceeded, the filler F-Number or A-Number limits are exceeded, PWHT is introduced or removed, the range of qualified thickness is exceeded or the welding process changes.

But, in reality, In companies conducting periodic WPS audits, the WPS library should be visited once a year, to ensure manufacturing practice continues to encompass the allowed variable ranges, especially after introducing new material suppliers, electrode manufacturers or shielding gas mixes.

Execute Your WPS at Scale — With Full Digital Traceability

Zhouxiang power industry robotic welding cells are built around your qualified WPS — with ±0.05 mm positioning accuracy, real-time parameter logging, and automatic pause on deviation. See how our systems deliver ASME-compliant production welding at scale.

See Power Industry Welding Robot Applications →

About This Guide

Zhouxiang has been designing and building robotic welding systems for the power generation and pressure vessel industries for over 30 years. The performance data cited in this guide — including the Henan Boiler Facility RT reject rate reduction from 9% to 1.8% — is drawn from documented customer installations operating under ASME BPVC-qualified WPS programmes. Our systems are certified to CE, ISO 9001:2015, ISO 3834-2, and ISO 10218-1. The standards comparison tables and parameter reference data are compiled from publicly available sources including ASME, AWS, CWB, and TWI; readers should verify all parameters against the current edition of the governing code for their specific application.

References & Sources

  1. AWS B2.1/B2.1M:2021 Welding Procedure and Performance Qualification — American Welding Society
  2. Standard Welding Procedure Specifications (SWPS) — American Welding Society
  3. ASME BPVC Section IX — Welding, Brazing, and Fusing Qualifications — American Society of Mechanical Engineers
  4. Typical Repair Rates for Welded Products — TWI (The Welding Institute)
  5. Welding Procedure Guide — Canadian Welding Bureau (CWB Group)
  6. AWS D1.1:2025 Structural Welding Code, Steel — Key Changes — ANSI
  7. Trends Shaping Welding Automation in 2026 — Pemamek (February 2026)